REVIEW 4 major objections 4 minor 71 references
Structural Relaxation Enables Millisecond Infrared Photodetection in Selenium Iodine Semiconductors
T0 review · 4 major / 4 minor · reviewed 2026-08-01 · deepseek-v4-flash
Pith's one-line read Structural aging of selenium–iodine turns a slow glassy photoconductor into a millisecond infrared detector.
desk verdict A potentially interesting empirical result (aged Se-I2 shows ms response) buried under a mechanism claim that is confounded and internally inconsistent. read the letter →
The pith
A machine-rendered reading of the paper's core claim, the machinery that carries it, and where it could break.
The reading
What carries the argument
The load-bearing mechanism is structural relaxation: the slow conversion of the metastable glassy Se–I2 network into a more ordered lamellar (partially crystalline) structure. This reduces the density of localized trap states that cause persistent photoconductivity. The fast device combines this relaxed material with a thin (~17 μm) lateral geometry on interdigitated platinum electrodes, which shortens carrier transit distances and gives uniform field; a vertical conductivity probe shows how iodine inhomogeneity degrades transport in thick films.
What would settle it
Fabricate the thin lateral device and test its response immediately after solidification, without months of aging and without extra iodine infusion; if it is already millisecond-fast, the speed-up is due to geometry or iodine content, not structural relaxation. Alternatively, track crystallinity (XRD or Raman) of the actual fast device over time and show that the speed increase tracks the crystallinity increase.
Extended reading notes
Core claim
The central claim is that the glass-to-crystal transition, not the selenium–iodine chemistry itself, sets the speed of Se–I2 photodetectors. Immediately after solidification the glassy network shows sluggish transport and persistent photoconductivity; after months of aging under reduced pressure the material orders into lamellae and the same material responds in 4.3 ms and tracks modulation up to 8 kHz. The paper also reports a vertical conductivity gradient in thick films, attributed to iodine loss during solidification, which explains why thick vertical devices are slow and motivates the thin lateral geometry.
Load-bearing premise
The paper attributes the dramatic speed-up to structural relaxation, but the fast device also differs from the slow one in thickness (17 μm vs 170 μm), electrode geometry (lateral interdigitated vs vertical stack), and iodine history (extra iodine infused during storage), so the improvement could come from any of these.
Editorial extensions
If this is right
- A cheap, solution-processable material can serve as an infrared detector at telecom (1550 nm) and visible wavelengths without cryogenic cooling.
- Post-fabrication aging — simply waiting — improves response speed by roughly three orders of magnitude, suggesting storage protocols matter for device performance.
- The vertical iodine gradient identified in thick films provides a doping lever for optimizing future Se–I2 devices.
- Demonstrated thermal imaging from 150 °C to 500 °C sources shows the material can form images in practical IR scenarios.
- The linear power dependence at 1550 nm versus ~0.5 exponent in the visible implies trap-free collection specifically in the infrared regime.
Reading between the lines
- If the mechanism is truly structural, then thermal annealing or seeding should accelerate crystallization from months to minutes, making the technology practical — a testable extension the paper does not perform.
- The same glass-relaxation logic may apply to other chalcogenide glasses with persistent photoconductivity, suggesting a broader design rule than Se–I2 alone.
- The iodine gradient could be engineered into a built-in field (graded doping) to improve carrier collection in vertical architectures, potentially recovering the simpler vertical geometry.
- The 0.4% photocurrent uniformity across lamellar morphology hints that grain-boundary engineering may not be needed for this material, lowering fabrication constraints.
Signed reviews
Editorial analysis
A structured set of objections, weighed in public.
Referee Report
Summary. The paper reports that solid-state selenium–iodine (Se-I2) evolves from a metastable glassy phase to an ordered lamellar structure during prolonged aging, and that this structural relaxation dramatically improves carrier transport. The authors present vertical devices showing slow bolometric response and a depth-dependent conductivity gradient, a slow lateral device with persistent photoconductivity, and an aged lateral device with ~17 μm film thickness on 10 μm interdigitated Pt electrodes that exhibits a 4.3 ms rise/fall time under 1550 nm illumination, stable photoresponse up to 8 kHz modulation, detectivities of ~10^8 Jones at 1550 nm and ~10^11 Jones in the visible, and infrared thermal imaging. The central claim is that the speedup is caused by structural ordering, not by changes in device geometry or iodine content.
Significance. If fully validated, the work would establish a solution-processable, low-cost infrared photodetector platform with millisecond response and demonstrate structural relaxation as a general strategy for engineering transport in selenium-based semiconductors. The authors are to be credited for fabricating multiple device architectures, performing long-term (12-month) monitoring, and demonstrating a practical imaging application. However, the manuscript's core causal claim—that aging-induced structural ordering, rather than changes in thickness, electrode geometry, or iodine stoichiometry, causes the performance improvement—is not convincingly isolated. An internal inconsistency between the reported 4.3 ms response time and the claimed flat response up to 8 kHz further undermines the quantitative headline claims. These issues are load-bearing and require additional experiments or careful re-analysis.
major comments (4)
- [§3.4, §3.5, §11.2] The central mechanism—that structural relaxation, not device geometry, causes the millisecond response—is not established because the slow and fast devices differ in multiple variables simultaneously. The slow vertical device is ~170 μm thick with ITO/Pt contacts; the slow lateral device is a 5 mm × 7 mm film; the fast device is ~17 μm thick on 10 μm interdigitated Pt and was stored with an additional 25 mg I2 for 4 weeks. No control experiment varies aging alone on the same geometry. Fig. S15 compares different devices, not the same device before/after aging. Without such a control, the speedup could be due to reduced thickness, lateral geometry, or iodine concentration.
- [Abstract and §3.5 (Fig. 4e,f)] The claim of a 4.3 ms response time is quantitatively inconsistent with the claim of stable operation up to 8 kHz. For a first-order system with τ=4.3 ms, the photocurrent amplitude at 8 kHz would be suppressed by a factor of ~1/(2πfτ) ≈ 1/216, not flat. Either the response time measurement or the 8 kHz bandwidth measurement is misinterpreted, or the two figures refer to different processes. The authors should provide a frequency-response curve and reconcile the time-constant and bandwidth.
- [Supplementary Section 2, Fig. S5; §3.5] No structural data are presented for the actual fast device. The only XRD pattern (Fig. S5) is from a solidified film on glass, not from the aged lateral device whose photoresponse is claimed to result from structural relaxation. Dark current trends in Figs. S1–S3 and the self-cited ChemRxiv (ref 13) are used to infer crystallization, but no time-resolved XRD or Raman measurement on the fast device is shown. This leaves the key causal step unverified.
- [Fig. S15 caption vs §11.2] The Fig. S15 caption attributes the fast response to 'removing the intercalated iodine and ageing,' whereas the fabrication section (§11.2) describes adding 25 mg I2 for iodine infusion. These statements are contradictory and bear directly on the proposed mechanism; please clarify whether iodine was added or removed.
minor comments (4)
- [Abstract] Detectivities are printed as '108 Jones' and '1011 Jones'; superscripts are missing and should be '10^8 Jones' and '10^11 Jones'.
- [§2, §3.4, §3.5] Several typographical inconsistencies: 'transfoms' in §3.5, 'Se–I₂' and 'SenI2' are used interchangeably, and the device area is stated as '1.5 mm×1.5 mm' in §11.2 while §3.5 mentions a different geometry. Please standardize notation.
- [§3.5] The text refers to 'Figure 5f' when discussing modulation frequency; this should be Figure 4f. Also, the response time is reported as both '4.32 ms' and '4.3 ms' in the same paragraph; please be consistent.
- [Supplementary Sections 1–2] The dark current evolution during crystallization is shown in Figures S1–S3, but these data are not referenced in the main text with explicit discussion of how they support the claimed structural relaxation. Please add cross-references and interpret the magnitude of the change.
Circularity Check
Device-speed data are measured, but the glassy-phase/structural-relaxation premise is imported from the authors' own ChemRxiv and then used to explain the speedup.
-
self citation load bearing
[Section 2 (Introduction), around ref. 13; echoed in Section 3.4]
"This previous study has also shown that upon cooling, liquid SeI2 forms a glassy phase13 that gradually recovers its crystalline character over time. ... Immediately after solidification from the melt, Se-I2 adopts a metastable glassy structure, as demonstrated by the thermal and structural characterization presented earlier.13"
The central causal claim is that aging transforms initially glassy Se-I2 into a more ordered structure and that this transformation causes the ~5000x speedup. But the paper presents no time-resolved structural measurement of the actual fast device; the initial glassiness and gradual recovery are asserted on the basis of ref. 13, the authors' own ChemRxiv preprint. The measured 4.3 ms response is then interpreted as evidence of this self-cited structural relaxation, so the explanatory premise is load-bearing self-citation rather than an independently verified structural observation.
full rationale
The headline empirical results — 4.3 ms rise/decay, 8 kHz operation, detectivity values — are measured and are not generated from fitted parameters, so there is no fitted-input-called-prediction circularity. The slow- versus fast-device comparison does confound aging with film thickness, lateral geometry, active area, and iodine exposure, but that is an experimental identification or correctness risk, not a definitional reduction to the paper's inputs. The only circularity-adjacent element is the structural-relaxation mechanism: the paper's premise that Se-I2 is initially glassy and gradually crystallizes is taken from the authors' own ChemRxiv (ref. 13), and the same premise is then invoked in §3.4 to attribute the speedup to structural relaxation. No independent time-resolved XRD or Raman data on the actual aged device anchors this step. Because the device-performance measurements themselves are self-contained and externally comparable, this is partial self-citation load-bearing rather than full circularity.
Assumptions & free parameters
free parameters (1)
- Photocurrent power-law exponent n =
n ≈ 1.1 (unaged vertical/lateral), n ≈ 0.5 (aged visible), n ≈ 1.0 (aged 1550 nm)
assumptions (4)
- domain assumption Solid Se-I2 consists of phase-separated selenium and iodine crystallites
- domain assumption Prolonged aging under reduced pressure promotes gradual structural relaxation/crystallization of the glassy phase
- domain assumption Detectivity is shot-noise-limited
- ad hoc to paper The response-speed improvement is caused by structural ordering, not by changes in device geometry or iodine content
Cite this review
Pith. "Pith review of Structural Relaxation Enables Millisecond Infrared Photodetection in Selenium Iodine Semiconductors." pith.science (2026). https://pith.science/paper/K7SER7JQ
@misc{pith2026260716054,
author = {Pith},
title = {Pith review of: Structural Relaxation Enables Millisecond Infrared Photodetection in Selenium Iodine Semiconductors},
year = {2026},
howpublished = {\url{https://pith.science/paper/K7SER7JQ}},
note = {Machine review of arXiv:2607.16054}
}
read the original abstract
The optoelectronic performance of amorphous and partially crystalline semiconductors is strongly governed by structural disorder, yet establishing direct correlations between structural evolution and carrier transport remains challenging. Here, we show that the solid state optoelectronic response of selenium iodine (SeI2) is dictated by its transformation from a metastable glassy phase into an ordered lamellar structure. Vertically resolved transport measurements reveal pronounced depth-dependent electrical conductivity within thick SeI2 films, arising from compositional and structural inhomogeneity developed during solidification. Immediately after solidification, the glassy SeI2 network exhibits sluggish carrier transport and persistent photoconductivity. Upon prolonged structural relaxation, however, the material undergoes significant transport enhancement, enabling millisecond-scale infrared photodetection with a response time of 4.3 ms, stable operation up to 8 kHz modulation frequency, and shot-noise-limited detectivities of 108 Jones at 1550 nm and 1011 Jones in the visible. Spatial photocurrent mapping demonstrates highly uniform carrier collection despite the self-assembled lamellar morphology, while infrared thermal imaging confirms practical imaging capability over a broad temperature range. These results establish structural relaxation as a powerful strategy for engineering carrier transport in selenium-based semiconductors and position SeI2 as a promising solution-processable platform for infrared photodetection and thermal imaging.
Figures
Reference graph
Works this paper leans on
-
[1]
Abstract: The optoelectronic performance of amorphous and partially crystalline semiconductors is strongly governed by structural disorder, yet establishing direct correlations between structural evolution and carrier transport remains challenging. Here, we show tha t the solid - state optoelectronic response of selenium–iodine (Se-I2) is dictated by its ...
-
[2]
Introduction: Infrared photodetectors have been studied for decades due to their wide -ranging applications in telecommunications 1–3, imaging 4–6, sensing, medical diagnostics 7, environmental and safety monitoring8, defense systems, and emerging quantum technologies9. Se-I2, a low melting point semiconductor10, has primarily been explored in its liquid ...
-
[3]
IISc” and (b) “SSCU
Result and Discussion: Structural characterization (Supplementary Section 2) confirms that, unlike the molten eutectic where selenium –iodine compounds have been reported, solid -state Se-I2 consists of distinct selenium and iodine phases, consistent with previous studies. 11,12 Establishing this structural distinction is important because the optoelectro...
-
[4]
Conclusion: In summary, we demonstrate that the optoelectronic performance of selenium -iodine (Se-I2) is intrinsically governed by its structural evolution during solidification and subsequent aging. While freshly solidified Se-I2 forms a metastable glassy structure that exhibits sluggish carrier transport and persistent photoconductivity, gradual struct...
-
[5]
set up experiments, collected data and wrote the manuscript
Author Contribution: B.J. set up experiments, collected data and wrote the manuscript
-
[6]
acknowledge funding support from Govt
Acknowledgements: B.J. acknowledge funding support from Govt. of India through Prime Research Fellowship and Research Grant with project code: PM/MHRD-19- 14871.03. B.J. acknowledge Anshu Pandey and Sushobhan Avasthi for insightful discussion. B.J. acknowledge Hridesh Kumar Gupta, for technical assistance I-V measurements and Ankur Bhaumik for thermal ima...
-
[7]
Flöry, N. et al. Waveguide-integrated van der Waals heterostructure photodetector at telecom wavelengths with high speed and high responsivity. Nat. Nanotechnol. 15, 118–124 (2020)
2020
-
[8]
Ma, P . et al. Fast MoTe2 Waveguide Photodetector with High Sensitivity at Telecommunication Wavelengths. ACS Photonics 5, 1846–1852 (2018)
2018
Show all 71 references
-
[9]
Hu, W. et al. Germanium/perovskite heterostructure for high-performance and broadband photodetector from visible to infrared telecommunication band. Light Sci. Appl. 8, 106 (2019)
2019
-
[10]
Wang, Y . et al. Silver telluride colloidal quantum dot infrared photodetectors and image sensors. Nat. Photonics 18, 236–242 (2024)
2024
-
[11]
Hwang, A. et al. Visible and infrared dual-band imaging via Ge/MoS 2 van der Waals heterostructure. Sci. Adv 7, eabj2521 (2021)
2021
-
[12]
Guo, J. et al. Type-printable photodetector arrays for multichannel meta-infrared imaging. Nat. Commun. 15, 5193 (2024)
2024
-
[13]
Ishigane, G. et al. Label-free mid-infrared photothermal live-cell imaging beyond video rate. Light Sci. Appl. 12, 174 (2023)
2023
-
[14]
Liu, M. et al. Uncooled near- to long-wave-infrared polarization-sensitive photodetectors based on MoSe2/PdSe2 van der Waals heterostructures. Nature Communications 16, 2774 (2025)
2025
-
[15]
Wang, Y . et al. Mid-infrared single-pixel imaging at the single-photon level. Nat. Commun. 14, 1073 (2023)
2023
-
[16]
Voss, L. F . et al. Selenium-iodide: A low melting point eutectic semiconductor. Appl. Phys. Lett. 113, 242103 (2018)
2018
-
[17]
& Milne, J
Gopal, M. & Milne, J. Spectroscopic Evidence for Selenium Iodides in CS2 Solution: Se3I2, Se2I2, and Sel2. Inorg. Chem vol. 31 https://pubs.acs.org/sharingguidelines (1992)
1992
-
[18]
Intra- and Intermolecular Correlations in Liquid Selenium-Halogen Systems
Kenji Maruyama, Yukinobu Kawakita, Makoto Yao, Hirohisa Endo & Masakatsu Misawa. Intra- and Intermolecular Correlations in Liquid Selenium-Halogen Systems. J. Physical Soc. Japan 60, 3032–3044 (1991)
1991
-
[19]
Jana, B. et al. SenI2: A Defect-Engineered Flowable Liquid Semiconductor. ChemRxiv https://doi.org/10.26434/chemrxiv.15002567/v1 (2026) doi:10.26434/chemrxiv.15002567/v1
2026 doi
-
[20]
& Drossinos, Y
Krausmann, E. & Drossinos, Y . A model of silver-iodine reactions in a light water reactor containment sump under severe accident conditions. Journal of Nuclear Materials 264, 113– 121 (1999)
1999
-
[21]
Tsarev, S. et al. Vertically stacked monolithic perovskite colour photodetectors. Nature 642, 592–598 (2025)
2025
-
[22]
Yang, T. et al. Van der Waals epitaxial growth and optoelectronics of large-scale WSe2/SnS2 vertical bilayer p-n junctions. Nat. Commun. 8, 1906 (2017)
1906
-
[23]
Li, H. M. et al. Ultimate thin vertical p-n junction composed of two-dimensional layered molybdenum disulfide. Nat. Commun. 6, 6564 (2015)
2015
-
[24]
Photogating in Low Dimensional Photodetectors
Hehai Fang & Weida Hu. Photogating in Low Dimensional Photodetectors. Advanced Science 4, 1700323 (2017)
2017
-
[25]
Hu, R. et al. Correlation between grain orientation and carrier concentration of poly-crystalline In2O3 thin film grown by MOCVD. J. Mater. Sci. 50, 1058–1064 (2015)
2015
-
[26]
Leshchenko, E. D. & Dubrovskii, V . G. Inhomogeneous dopant distribution in III–V nanowires. Semiconductors 51, 1427–1430 (2017)
2017
-
[27]
Kim, Y . S. et al. Thickness-dependent bulk properties and weak antilocalization effect in topological insulator Bi2Se3. Phys. Rev. B 84, 073109 (2011)
2011
-
[28]
Jiang, C. S. et al. Imaging hole-density inhomogeneity in arsenic-doped CdTe thin films by scanning capacitance microscopy. Solar Energy Materials and Solar Cells 209, 110468 (2020)
2020
-
[29]
Iodine Chemistry and Applications
Tatsuo Kaiho. Iodine Chemistry and Applications. vol. ISBN:9781118909911 (2014)
2014
-
[30]
Julie Euvrard, Yanfa Yan & David B. Mitzi. Electrical doping in halide perovskites. nature reviews materials 6, 531–549 (2021)
2021
-
[31]
Point defect engineering in thin-film solar cells
Ji Sang Park, Sunghyun Kim, Zijuan Xie & Aron Walsh. Point defect engineering in thin-film solar cells. Nat. Rev. Mater. 3, 194–210 (2018)
2018
-
[32]
Gap States in Amorphous Selenium: What Are the Atomic Structures? Phys
Keiji Tanaka & Tamihiro Gotoh. Gap States in Amorphous Selenium: What Are the Atomic Structures? Phys. Status Solidi B 262, 2400458 (2025)
2025
-
[33]
Golden & Vassiliy Lubchenko
Alexey Lukyanov, Jon C. Golden & Vassiliy Lubchenko. Structural Origin of the Midgap Electronic States and the Urbach Tail in Pnictogen-Chalcogenide Glasses. J. Phys. Chem. B 122, 8082– 8097 (2018)
2018
-
[34]
D. V . Lang & R. A. Logan. Large-Lattice-Relaxation Model for Persistent Photoconductivity in Compound Semiconductors. Phys. Rev. Lett. 39, 635 (1977)
1977
-
[35]
Marshall I. Nathan. Persistent photoconductivity in AlGaAs/GaAs modulation doped layers and field effect transistors: A review. Solid. State. Electron. 29, 167–172 (1986)
1986
-
[36]
Photoelectric Properties of Amorphous Selenium Thin Films Deposited by Thermal Evaporation
Zhadyra Toreniyaz et al. Photoelectric Properties of Amorphous Selenium Thin Films Deposited by Thermal Evaporation. Chalcogenide Letters 23, (2026)
2026
-
[37]
M., Hou, C., Liu, L
Liao, Z. M., Hou, C., Liu, L. P . & Yu, D. P . Temperature dependence of photoelectrical properties of single selenium nanowires. Nanoscale Res. Lett. 5, 926–929 (2010)
2010
-
[38]
Zhang, M. et al. High-Performance Photodiode-Type Photodetectors Based on Polycrystalline Formamidinium Lead Iodide Perovskite Thin Films. Sci. Rep. 8, 11157 (2018)
2018
-
[39]
Wei, Y ., Lan, C., Zhou, S. & Li, C. Recent Advances in Photodetectors Based on Two- Dimensional Material/Si Heterojunctions. Applied Sciences 13, 11037 (2023)
2023
-
[40]
Cao, F ., Liu, L. & Li, L. Short-wave infrared photodetector. Materials Today 62, 327–349 (2023)
2023
-
[41]
& Sargent, E
Konstantatos, G. & Sargent, E. H. Nanostructured materials for photon detection. Nat. Nanotechnol. 5, 391–400 (2010)
2010
-
[42]
Huang, W. et al. Enhanced Photodetection Properties of Tellurium@Selenium Roll-to-Roll Nanotube Heterojunctions. Small 15, 1900902 (2019)
2019
-
[43]
Zhang, H. et al. Broadband photodetector based on vapor-deposited selenium self-supporting films. Ceram. Int. 48, 27750–27757 (2022)
2022
-
[44]
K., Prakash, R., Kumar, N
Chaudhary, V ., Pandey, R. K., Prakash, R., Kumar, N. & Singh, A. K. Highly aligned and crystalline poly(3-hexylthiophene) thin films by off-center spin coating for high performance organic field- effect transistors. Synth. Met. 258, 116221 (2019)
2019
-
[45]
Noriega, R. et al. A general relationship between disorder, aggregation and charge transport in conjugated polymers. Nat. Mater. 12, 1038–1044 (2013)
2013
-
[46]
Amorphous selenium and its alloys from early xeroradiography to high resolution X-ray image detectors and ultrasensitive imaging tubes
Safa Kasap et al. Amorphous selenium and its alloys from early xeroradiography to high resolution X-ray image detectors and ultrasensitive imaging tubes. Physica Status Solidi b 246, 1794–1805 (2009)
2009
-
[47]
Modeling Dark Current Conduction Mechanisms and Mitigation Techniques in Vertically Stacked Amorphous Selenium-Based Photodetectors
Le Thanh Triet Ho et al. Modeling Dark Current Conduction Mechanisms and Mitigation Techniques in Vertically Stacked Amorphous Selenium-Based Photodetectors. ACS Appl. Electron. Mater. 3, 3538–3546 (2021)
2021
-
[48]
Xu, D. et al. Deciphering photocurrent mechanisms at the nanoscale in van der Waals interfaces for enhanced optoelectronic applications. Sci. Adv 11, 7614 (2025)
2025
-
[49]
Yin, J. et al. Selectively enhanced photocurrent generation in twisted bilayer graphene with van Hove singularity. Nat. Commun. 7, (2016)
2016
-
[50]
Thantsha, E.Q.B
N.M. Thantsha, E.Q.B. Macabebe, F .J. Vorster & E.E. van Dyk. Opto-electronic analysis of silicon solar cells by LBIC investigations and current–voltage characterization. Physica B Condens. Matter 404, 4445–4448 (2009)
2009
-
[51]
Probing Photocurrent Nonuniformities in the Subcells of Monolithic Perovskite/Silicon Tandem Solar Cells
Zhaoning Song et al. Probing Photocurrent Nonuniformities in the Subcells of Monolithic Perovskite/Silicon Tandem Solar Cells. J. Phys. Chem. Lett. 7, 5114–5120 (2016). Structural Relaxation Enables Millisecond Infrared Photodetection in Selenium–Iodine Semiconductors Biman Ja...
2016
-
[52]
The picture on the left shows the Se-I2 material in liquid state
Dark Current and Photocurrent Variation upon Crystallization: Figure S1: Dark current variation with crystallization of the material. The picture on the left shows the Se-I2 material in liquid state. The picture on the right shows the material after allowing it to crystallize ...
-
[53]
The porous structure of the Se-I2 is obvious from the SEM image (Figure S 4a-b)
Structural Characterizations: 2.1 SEM Image and Elemental Mapping: Figure S3: (a-b) SEM image of typical film on silicon and (c) and (d) energy dispersive X-ray spectra EDS elemental mapping for selenium and iodine respectively for the area shown in (b). The porous structure o...
-
[54]
The mixture was then immediately decanted on the substrate
Preparing Film of Se-I2 For Vertical Devices: 64 mg of Selenium powder and 200 mg of molecular Iodine was mixed and heated up in a closed argon environment. The mixture was then immediately decanted on the substrate. A Si wafer was placed on top of the liquid to ensure a flat ...
-
[55]
Figure S 8: (a) Vertical stack device geometry designed with an extra layer of Ti2 as an electron transport layer
Vertical Device Response: Figure S7: Comparison of two vertical devices: I-V characteristics of vertical stack device where (a) Ag paste is used directly on top of Se-I2 layer and (b) 150 nm Platinum layer is used before making electrical contact with Ag paste on top of it. Fi...
-
[56]
Photodetector device parameters: 5.1. Photocurrent to Dark Current Ratio: The rise in current flowing through a photodetector upon excitation with light is called the photocurrent 𝐼𝑝ℎ𝑜𝑡𝑜 𝐼𝑑𝑎𝑟𝑘 = 𝐼𝑏𝑟𝑖𝑔ℎ𝑡−𝐼𝑑𝑎𝑟𝑘 𝐼𝑑𝑎𝑟𝑘 ………………………………………….……………..………………….(1) Where 𝐼𝑝ℎ𝑜𝑡𝑜 is the photoc...
-
[57]
Horizontal Slow Device Characteristics: Figure S9: Photo response of the large area horizontal devices (5 mm × 7 mm) covering the at different power illumination of 1550 nm source as indicated in the Figures (a-h). The background has been subtracted to omit the continuous drif...
-
[58]
The power densities are mentioned in legends
Characterization of the Faster Horizontal Device: 7.1 Thickness of the Device: Figure S11: Tilted SEM image showing the thickness of the film ~17 𝜇m 7.2 I-V Sweeps of Horizontal Device: Figure S12: I-V characteristics of a typical horizontal Se-I2 device with different power o...
-
[59]
(a-c) I-V characteristics of a typical horizontal device measured at 300 K, 200 K and 35 K respectively
Low Temperature Photoresponse and I -V Sweeps at Different Powers: Figure S 16: The temperature dependence of photo response . (a-c) I-V characteristics of a typical horizontal device measured at 300 K, 200 K and 35 K respectively. (d) The dark current and the percentage of ph...
-
[60]
The ceramics was open to emission to the parabolic mirror in the place of the letters
Thermal Imaging Set-up: Figure S17: Imaging using Horizontal photodetector: (a) The set up for imaging of is made with a hot plate covered with aluminum foil and the foil was cut with the letters desired to be imaged. The ceramics was open to emission to the parabolic mirror i...
-
[61]
Experimental: 11.1. Synthesis and Basic Characterizations: The material has been made by adding 0.8 mmol (200 mg) iodine (I2) to 0.8 mmol (64 mg) of Selenium (Se) powder in a round bottom flask in inert condition (Argon in Schlenk line ), gently heating it up to 70 oC to liqui...
-
[62]
& Zheng, Q
Liu, Y., Xu, Z. & Zheng, Q. The interlayer shear effect on graphene multilayer resonators. Journal of the Mechanics and Physics of Solids 59, 1613–1622 (2011)
2011
-
[63]
Wang, W. et al. Measurement of the cleavage energy of graphite. Nat Commun 6, 7853 (2015)
2015
-
[64]
& Luo, J
Li, J., Li, J. & Luo, J. Superlubricity of Graphite Sliding against Graphene Nanoflake under Ultrahigh Contact Pressure. Advanced Science 5, 1800810 (2018)
2018
-
[65]
I., Ullah, Z., Haider, S
Sonil, N. I., Ullah, Z., Haider, S. & Ahmad, W. Flexible UV photodetector based on graphite/titanium dioxide through facile transfer of pencil drawn graphite films on desired substrates. Ceramics International 50, 37057–37066 (2024)
2024
-
[66]
& Zhu, Y
Xu, F., Lu, W. & Zhu, Y. Controlled 3D Buckling of Silicon Nanowires for Stretchable Electronics. ACS Nano 5, 672–678 (2011)
2011
-
[67]
M., Jiang, H., Huang, Y
Sun, Y., Choi, W. M., Jiang, H., Huang, Y. Y. & Rogers, J. A. Controlled buckling of semiconductor nanoribbons for stretchable electronics. Nature Nanotech 1, 201–207 (2006)
2006
-
[68]
Yao, L. et al. High‐efficiency stretchable organic light‐emitting diodes based on ultra‐ flexible printed embedded metal composite electrodes. InfoMat 5, e12410 (2023)
2023
-
[69]
Posar, J. A. et al. Polymer Photodetectors for Printable, Flexible, and Fully Tissue Equivalent X‐Ray Detection with Zero‐Bias Operation and Ultrafast Temporal Responses. Adv Materials Technologies 6, 2001298 (2021)
2021
-
[70]
Kim, H. et al. A Flexible and Wavelength‐Designable Polymer Light‐Emitting Diode Employing Sandwich‐Encapsulation for Wearable Skin Rejuvenation Photomedicine. Adv Materials Inter 8, 2100856 (2021)
2021
-
[71]
Kaltenbrunner, M. et al. Ultrathin and lightweight organic solar cells with high flexibility. Nat Commun 3, 770 (2012)
2012
Reviewed August 1, 2026 · model on record in the stance chip above.